Database of properties for steel and alloy materials worldwide.

 
Showing posts with label UN Standard. Show all posts
Showing posts with label UN Standard. Show all posts

X2CrNiMoN22-5-3 ( 1.4462 ): COMPOSITION, PROPERTIES AND EQUIVALENT STEELS

Grade :     X2CrNiMoN22-5-3
    Number:     1.4462
    Standard: EN 10088 - 2 : 2005   Stainless steels. Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
EN 10088 - 3 : 2005   Stainless steels. Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes
    Classification:     Austenitic-ferritic stainless steels - standard grade

X30Cr13 (1.4028 ): COMPOSITION, PROPERTIES AND EQUIVALENT STEELS

    Grade :

    X30Cr13

    Number:

    1.4028

    Standard:

EN 10088 - 2 : 2005   Stainless steels. Technical delivery conditions for sheet/plate and strip of corrosion resisting steels for general purposes
EN 10088 - 3 : 2005   Stainless steels. Technical delivery conditions for semi-finished products, bars, rods, wire, sections and bright products of corrosion resisting steels for general purposes

    Classification:

    Martensitic stainless steels - standard grade

 

Chemical composition % of the ladle analysis   of grade   X30Cr13 (1.4028)

Tighter carbon ranges may be agreed at the time of enquery and order.
Particular ranges of sulphur content may provide improvement of particular properties. For machinability a controlled sulphur content of 0.015 % to 0.030% is recommended and permitted. For weldability, a controlled sulphur content of 0.008 % to 0.030 % is recommended and permitted. For polishability, a controlled sulphur content of 0.015 % max is recommended.

Elements not listed in this table shall not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast.

 

C

Si

Mn

P

S

Cr

0.26 - 0.35

max   1

max   1.5

max   0.04

max   0.015

12 - 14

 

Equivalent grades of grade   X30Cr13 (1.4028)

USA
-

Japan
JIS

France
AFNOR

England
BS

Sweden
SS

Poland
PN

Russia
GOST

420

SUS420J2

Z33C13

420S45

2304

3H13

3H14

30KH13

Mechanical Properties

Quantity

Value

Unit

Young's modulus

200000 - 200000

MPa

Tensile strength

650 - 880

MPa

Elongation

8 - 25

%

Fatigue

275 - 275

MPa

Yield strength

350 - 550

MPa

Physical Properties

Quantity

Value

Unit

Thermal expansion

10 - 10

e-6/K

Thermal conductivity

25 - 25

W/m.K

Specific heat

460 - 460

J/kg.K

Melting temperature

1450 - 1510

°C

Density

7700 - 7700

kg/m3

Resistivity

0.55 - 0.55

Ohm.mm2/m

Environmental Data

Quantity

Value

Unit

Eco indicator 95

3.475

mPt

EPS

4660

mELU

Ex (in) / Ex (out)

3.69770580296896

MJ/MJ

GER

24.6

MJ

Raw materials input

3.35448049509064

kg

Solid

0.0107959

kg

Eco indicator 99

0.119

Pt

Environmental remarks

Important producers of Stainless steels are the US (14%), Germany (9%), CIS (10%),and France (6%). The average scrap supply is 20%. See for the environmental aspects the individual alloy metals data.

General

Remarks

 (Fe rest, C 0.30, Cr 13.0, Si <1.0, Mn <1.0 (wt.%))

 